1. Definition & Core Purposes of Pre-Crushing
Pre-crushing (coarse crushing / primary crushing) is the front-end crushing process for bulk calcined petroleum coke / needle coke before fine jet milling, including multi-stage crushing + initial sieving + impurity removal.
Core objectives:
- Reduce 50–200 mm bulk coke lumps into uniform small particles, stable feeding for downstream roller mill / jet mill, prevent equipment blockage and uneven grinding load.
- Expose wrapped mineral gangue, refractory brick debris and metal foreign bodies for front-end magnetic separation & screening removal.
- Shorten subsequent fine grinding time, narrow particle size distribution (PSD), reduce ultra-fine dust generation and control BET surface area.
- Create uniform particle gaps for later pitch kneading homogenization, improve pitch coating uniformity and tap density of granulated precursors.
Raw feed: Calcined petroleum coke / needle coke (bulk lump size 50–200 mm, moisture ≤3.0% after calcination cooling).
2. Full Pre-Crushing Process Flow Standard
Raw coke feeding → primary magnetic iron removal → jaw primary coarse crushing → vibrating initial sieving → secondary hammer/roller medium crushing → secondary magnetic separation → secondary sieving → qualified pre-crushed intermediate stock silo
All equipment contact surfaces adopt zirconia ceramic / PU lining to avoid secondary iron contamination.
3. Tiered Particle Size Standard (Critical Technical Index)
3.1 Primary Jaw Coarse Crushing (1st Stage Pre-Crushing)
- Incoming lump size: 50–200 mm bulk coke
- Discharge target particle size: All particles ≤10 mm
- Oversize control standard: Material >10 mm residue on screen ≤2.0% by mass; oversized lumps loop back to jaw crusher for re-crushing
- Gap adjustment: Jaw discharge gap set 8–12 mm according to raw coke hardness
- Supporting equipment: Permanent magnetic separator at discharge port to remove steel fragments from calcination furnace lining
3.2 Secondary Medium Crushing (2nd Stage Pre-Crushing, Mandatory for Battery-Grade)
Adopt sealed hammer crusher or double roller crusher after primary sieving to further reduce particle size:
- Target finished pre-crushed particle size: All particles ≤5 mm (0–5 mm)
- Optimal main fraction distribution: 1–3 mm accounts for 60–75% of total mass
- Fine powder control: Fraction <0.5 mm ≤10% (excess fine powder causes high BET after fine milling, low initial Coulombic efficiency)
- Oversize index: Residue >5 mm after secondary sieving ≤1.0%
3.3 Unified Pre-Crushed Finished Particle Acceptance Standard
| Item | Industrial Standard for Artificial Graphite Coke Pre-Crushing |
|---|---|
| Maximum particle size Dmax | ≤5 mm |
| Main particle fraction (1–3 mm) | 60–75 wt% |
| Superfine fraction (<0.5 mm) | ≤10 wt% |
| Oversize (>5 mm) residue rate | ≤1.0% |
| Particle size span uniformity | No large lump segregation, uniform grading |
4. Equipment Selection & Anti-Contamination Mandatory Requirements
4.1 Standard Pre-Crushing Equipment Matching
- Primary crushing: Jaw crusher (all lining plates zirconia / high manganese non-magnetic alloy)
- Secondary crushing: Double roller crusher (low dust generation, controllable particle grading) or closed hammer mill (for high-hardness needle coke)
- Screening: 10 mesh (2.0 mm) + 5 mesh (4.0 mm) double-layer linear vibrating screen, 316L stainless steel anti-wear mesh
- Magnetic separation: Double-stage strong magnetic separator (magnetic field strength ≥12000 Gs) before & after crushing
4.2 Strict Anti-Iron Contamination Rules (Battery-Grade Hard Requirement)
- No carbon steel contact liners inside crushing cavity; replace worn metal liners immediately to avoid iron powder mixing into coke.
- Two-stage magnetic iron removal:
- Front feeding magnetic separator: Remove calcination furnace refractory iron scraps, conveying equipment wear debris
- Post-crushing magnetic separator: Eliminate iron micro-particles generated by crusher liner friction
- Control target: Total iron impurity of pre-crushed coke ≤8 ppm before fine milling
5. Raw Material Pre-Conditioning Requirements Before Crushing
5.1 Moisture Control
- Calcined coke incoming moisture ≤3.0%
- If moisture >3.0%, equip low-temperature rotary dryer (100–130°C nitrogen hot air) before crushing to eliminate screen mesh blinding and coke agglomeration.
- Pre-crushed finished material moisture stabilized ≤2.0% before entering homogenization silo.
5.2 Foreign Body Removal Standard
- Manual pre-sorting before feeding: Remove refractory brick, plastic, wood, stone gangue mixed in coke lumps.
- After two-stage crushing + screening: No visible hard rock, metal blocks, organic foreign bodies in pre-crushed coke.
- Foreign body inspection limit: ≤2 visible impurities per 100 kg pre-crushed material.
5.3 Raw Coke Batch Homogenization Before Crushing
Stack multi-batch calcined coke by ash, volatile content, true density; cross-layer reclaiming homogenization ≥12 h to avoid large performance fluctuation of pre-crushed material from different batches.
6. Operation & Process Control Parameters
- Feeding speed: Uniform continuous feeding, avoid instantaneous over-feeding causing crusher cavity blockage; install buffer silo + quantitative screw feeder.
- Crushing temperature: Closed nitrogen circulation inside crusher to isolate air; material surface temperature ≤150°C to prevent coke surface oxidation.
- Circulation re-crushing rule: All oversize particles >5 mm automatically return to secondary roller crusher via belt conveyor closed loop, no manual open circulation.
- Sampling frequency: Test particle size distribution every 30 min at secondary screening discharge port; record oversize residue rate, fine powder proportion.
7. Post Pre-Crushing Intermediate Storage Requirements
- Sealed nitrogen-blanketed silo storage, internal RH ≤35% to prevent moisture re-absorption.
- Pre-crushed coke stored in silo for ≥8 h circulation homogenization to eliminate particle size segregation (large/small particle layering).
- Silo discharge magnetic separation again before feeding to jet mill fine grinding station.
8. Common Unqualified Defects & Adjustment Standards
- Excess oversize >5 mm (residue >1.0%)
- Causes: Excessive crusher discharge gap, fast feeding speed, worn screen mesh
- Solutions: Narrow roller/jaw gap, reduce feeding rate, replace deformed screen cloth
- Too much superfine powder <0.5 mm (>10%)
- Causes: Over-crushing, too small roller gap, long hammer impact time
- Solutions: Widen secondary roller gap, reduce hammer mill rotation speed
- Excess iron impurities (>8 ppm)
- Causes: Worn metal liners, insufficient magnetic separator magnetic strength
- Solutions: Replace ceramic lining, upgrade high-strength magnetic separator, increase magnetic separation times
- Mesh blinding during screening
- Causes: Raw coke moisture >3.0%, static agglomeration
- Solutions: Pre-dry coke, install ultrasonic anti-blocking vibration device on screen
9. Full Pre-Crushing Standard Summary
- Two-stage crushing flow: Jaw primary crush (≤10 mm) → roller secondary crush (final Dmax ≤5 mm).
- Grading target: 1–3 mm main fraction 60–75%, fine powder <0.5 mm ≤10%, oversize >5 mm ≤1.0%.
- Hard quality limits: Fe impurity ≤8 ppm, moisture ≤2.0%, no metal/rock foreign bodies.
- Supporting configuration: Double-stage magnetic separation, full non-magnetic ceramic lining, closed nitrogen circulation, automatic oversize loop re-crushing.
Qualified pre-crushed coke with uniform particle grading lays a foundation for narrow PSD fine grinding, stable kneading homogenization and consistent electrochemical performance of finished artificial graphite anode. All pre-crushing system design complies with JACAN full-line low-contamination coke pretreatment standards.